Measuring out of Plane Elastic Moduli in Solid Bleached Board
Ultrasonic pulse velocity measuring C33 compressional stiffness and Gxz shear modulus provides exact non-destructive Z-plane elastic moduli for SBS board.

Sonic

Acoustic Time of Flight Measurements across Sheet Thickness
High-frequency stress wave propagation offers direct access to out-of-plane elastic parameters without introducing damage or the compliance errors inherent to adhesive mounting tapes. Solid bleached board consists of several plies of refined chemical pulp pressed and calendered into a dense sheet. Gripping that structure in static Z-tensile fixtures captures the bond strength at failure instead of true elastic behavior, whereas ultrasonic transit times isolate early stiffness long before micro-yield sets in.
Piezoelectric transducers operating between 1 MHz and 5 MHz send longitudinal compression waves directly through the sheet thickness. Under ISO 22484 and TAPPI T 577 protocols, these tools establish the longitudinal out-of-plane stiffness coefficient by pressing upper and lower transducers against the board at controlled contact loads. The instrument records the microsecond transit delay between emission and reception across the caliper.
Solid bleached board exhibits an out-of-plane Young’s modulus of 150 MPa to 350 MPa when tested under ISO 187 standard atmosphere at 23 degrees Celsius and 50 percent relative humidity.
Sound velocity combined with sheet density yields the elastic stiffness tensor component. Out-of-plane compressional stiffness scales directly with the square of ultrasonic wave speed.
- Longitudinal Wave Velocity ~ Pulses travel through the thickness dimension to determine compressional elastic response perpendicular to outer clay coatings.
- Polarized Shear Wave Velocity ~ Transverse pulses align with machine direction and cross direction to isolate out-of-plane shear stiffness components.
- Apparent Sheet Density ~ Grammage divided by optical thickness provides the mass per unit volume needed to convert acoustic speed into stiffness units.
- Acoustic Delay Compensation ~ Buffer rods absorb excess transducer ringing and isolate signal phase shifts occurring at contact surfaces.
Standard double-sided tape tests such as TAPPI T 541 lump the board’s structural stiffness together with the elastomeric give of the adhesive. Sound propagation avoids that compliance entirely. In high-density solid bleached sulfate, the acoustic pulse traverses the sheet in under one microsecond, meaning timer circuits require nanosecond resolution to separate subtle furnish differences.
Relying on static Z-tensile break forces rather than dynamic acoustic moduli leaves packaging converters guessing about elastic crease recovery.

Acoustic Stiffness Calculation Fundamentals
Density scales raw acoustic velocity into true elastic stiffness, defining the compressional modulus across the sheet thickness.
Transit time converts directly to the out-of-plane elastic stiffness matrix component:
C33 = density (caliper / transit_time)^2
In this formulation, C33 represents the Z-direction compressional stiffness in megapascals, density is expressed in grams per cubic centimeter, caliper is measured in micrometers, and transit time is recorded in microseconds after subtracting buffer delay.
Because out-of-plane Poisson cross-coupling in orthotropic sheets is minimal, C33 stands in reliably for the out-of-plane Young’s modulus Ez. Shear moduli use the same relationship with transverse wave arrivals.
Gxz = density (caliper / shear_transit_time_MD)^2
Gyz = density (caliper / shear_transit_time_CD)^2
Calculating transit times accurately hinges on clean wavefront identification. Digital oscilloscopes key off the first zero-crossing or peak amplitude to prevent phase shift errors.

Orthotropy

Constitutive Matrix for Virgin Chemical Pulp Webs
Fiber orientation set during headbox delivery and table drainage establishes a pronounced three-dimensional symmetry. Solid bleached board functions as an orthotropic material with three distinct axes: machine direction (1), cross direction (2), and sheet thickness (3). Nine independent elastic constants define the complete stiffness matrix governing how cartons deform under complex loads.
In-plane moduli Ex and Ey routinely exceed out-of-plane modulus Ez by more than an order of magnitude. Machine-direction fiber orientation yields Ex values between 5000 MPa and 9000 MPa in premium bleached sulfate, while out-of-plane stiffness Ez hovers between 150 MPa and 350 MPa because through-thickness bonds rely only on sparse hydrogen networks. Out-of-plane shear moduli Gxz and Gyz drop further still, generally falling between 80 MPa and 180 MPa.
| Elastic Constant | Physical Axis Mapping | Typical SBS Range | Primary Furnish Driver |
|---|---|---|---|
| Ex (E1) | Machine Direction Tensile Modulus | 6500 – 8500 MPa | Softwood fiber jet-to-wire speed ratio |
| Ey (E2) | Cross Direction Tensile Modulus | 3000 – 4200 MPa | Cross-machine fiber orientation profile |
| Ez (E3) | Out-of-Plane Tensile Modulus | 180 – 320 MPa | Z-directional refining and wet pressing density |
| Gxy (G12) | In-Plane Shear Modulus | 1800 – 2400 MPa | Inter-fiber bond density and drying strain |
| Gxz (G13) | MD-ZD Out-of-Plane Shear Modulus | 110 – 160 MPa | Softwood/hardwood ratio in middle plies |
| Gyz (G23) | CD-ZD Out-of-Plane Shear Modulus | 90 – 140 MPa | Fibrillation level and Z-plane fiber entanglements |
| vxy (v12) | In-Plane Poisson Ratio | 0.32 – 0.40 | Fibrillar network strain distribution |
| vxz (v13) | MD-ZD Out-of-Plane Poisson Ratio | 0.01 – 0.04 | Low thickness compliance constraint |
| vyz (v23) | CD-ZD Out-of-Plane Poisson Ratio | 0.01 – 0.03 | Transverse ply swelling capability |
Out-of-plane Poisson ratios vxz and vyz run exceptionally low relative to in-plane numbers; pulling a board coupon in tension produces almost no measurable contraction through its thickness. For standard bleached board, C33 and Ez diverge by less than two percent, which lets ultrasonic longitudinal modulus serve directly as out-of-plane Young’s modulus in converting models.

Multi-Ply Structural Symmetry Effects
Modern board machines build solid bleached grades by couching two to four wet pulp webs on the wire. Outer plies carry highly refined bleached softwood kraft to guarantee smooth, durable surfaces for print and creasing, while middle plies use bleached hardwood or high-yield mechanical pulps to add bulk. These through-thickness modulus steps shift the neutral axis during bending.
Substantial out-of-plane compliance lets outer plies slide over core layers when bent around tight radii. Low Gxz and Gyz values foster this controlled internal shear during folding, protecting coated top liners from tension checks on high-speed packaging lines. Just how dynamic shear coupling behaves at multi-ply interfaces under rapid impact remains an open problem in paper physics.

Probe

Transducer Contact Pressure and Caliper Measurement Propagation
Accurate caliper measurement controls the fidelity of every calculated out-of-plane constant. Thickness enters modulus equations as a squared term in velocity and linearly in density, meaning calculated modulus scales directly with measured thickness over the square of transit time. A minor discrepancy in caliper quickly skews the output.
Mechanical micrometers with rigid steel anvils sink into paper under dead-weight loads. Standard ISO 534 testing exerts 50 kPa to 100 kPa of contact pressure, compressing bulky core plies on contact. These compressed thickness readings shorten the assumed path length and distort calculated density.
Optical displacement gauges and soft-faced ultrasonic heads avoid anvil sink entirely.
| Measurement Method | Applied Pressure | Measured Caliper | Calculated Density | Calculated Ez Modulus |
|---|---|---|---|---|
| ISO 534 Dead-Weight Micrometer | 100 kPa | 338 micrometers | 0.828 g/cm3 | 210 MPa |
| TAPPI T 411 Mechanical Gauge | 50 kPa | 344 micrometers | 0.814 g/cm3 | 228 MPa |
| Laser Optical Displacement Sensor | 0 kPa | 352 micrometers | 0.795 g/cm3 | 248 MPa |
| Soft Transducer Contact Assembly | 10 kPa | 350 micrometers | 0.800 g/cm3 | 242 MPa |
Contact pressure also changes the actual acoustic path. Squeezing the sheet compacts internal voids, shortening pulse travel time and inflating calculated stiffness. Enforcing consistent transducer loading stops borderline, low-density lots from slipping past specification limits.

Zero-Point Time Delay Calibration Sequence
Transducer faces and internal delay buffers add baseline electronic and acoustic lags. Calibrating the zero point isolates these fixture delays from true transit times through the sheet.
- Clean transducer contact faces with isopropyl alcohol to remove dry chemical size and paper dust.
- Apply a uniform thin layer of synthetic ultrasonic couplant fluid across both contact surfaces.
- Bring upper and lower transducers into direct face-to-face contact under standard 10 kPa pneumatic load.
- Record the electronic time delay baseline value on the digital signal processing receiver.
- Insert precision steel calibration gauge blocks of known thickness and acoustic velocity to verify system linearity.
- Measure sample pulse transit time and subtract recorded system delay baseline before processing modulus output.
Surface fiber compression under transducer contact pressure regularly distorts routine caliper checks, shifting reported numbers without altering underlying pulp quality. Precision testing demands absolute standard compliance for contact load.
Compliance with TAPPI T 577 standard method fixes the ultrasonic contact pressure at 0.1 MPa to prevent structural compaction of low-density bleached sulfate plies.

Delamination

Structural Failure Mechanics in Carton Creasing
Converting solid bleached board into packaging blanks requires precise mechanical scoring along fold lines. Scoring dies press a metal rule into the board substrate, forcing it into a female matrix groove. This localized deformation creates a controlled zone of internal delamination within the middle plies.
High out-of-plane elastic modulus Ez resists initial creasing rule penetration, raising required creasing forces.
Failure occurs when out-of-plane shear stresses exceed internal bond strength. Adequate delamination splitting permits the inner plies to bulge inward during a 90-degree or 180-degree fold. Controlled internal sliding prevents outer print coatings from cracking under tensile tension.
Boards with exceptionally high Ez and Gxz values resist internal shear failure, forcing bending stresses into outer liner surfaces where disastrous visible cracking develops.
Proper multi-ply furnish design maintains distinct elastic properties across individual plies.
- Top Coating Layer ~ High elastic modulus prevents surface cracking and provides smooth printing performance under heavy ink coverage.
- Top Bleached Chemical Kraft Ply ~ High in-plane tensile stiffness absorbs bending tension without premature surface rupture during score folding.
- Bulk Building Middle Plies ~ Lower out-of-plane elastic modulus and lower shear modulus promote controlled internal ply separation within the crease matrix.
- Bottom Bleached Chemical Kraft Ply ~ High strain to failure accommodates compression bulging inside the folded carton corner.
Internal bond strength measured by Scott Bond testing correlates loosely with ultimate tensile fracture force but fails to predict dynamic elastic deformation. Out-of-plane shear modulus Gyz dictates how readily inner plies delaminate under high-speed creasing impacts. Converting lines running at 300 meters per minute generate stress wave frequencies matching laboratory ultrasonic test bands.

Score Stiffness Ratio Optimization
Fold performance evaluation compares the bending resistance of an uncreased sheet to the bending resistance of a creased fold line. The ratio defines score stiffness reduction.
High out-of-plane shear modulus hinders score formation. A stiff inner core prevents ply sliding, producing high score stiffness ratios above 60 percent. Target converting performance requires score ratios between 35 percent and 50 percent.
Lower values indicate easy bending without pack distortion.
Higher middle ply hardwood content lowers out-of-plane shear modulus without degrading outer surface strength. Lowering shear modulus allows clean internal delamination under low creasing force.
Higher hardwood kraft ratios in the center ply increase z-directional compressibility while reducing dynamic shear stiffness.
Fibers inside soft middle plies separate cleanly along secondary cell wall layers; hardwood fiber networks yield under out-of-plane shear stress, allowing controlled delamination that preserves outer liner integrity.

Conditioning

Moisture and Temperature Equilibrium Dynamics
Cellulose fibers absorb ambient moisture readily, altering structural hydrogen bonding and inter-fiber friction. Water molecules act as plasticizers inside the amorphous regions of cell wall polymers. Increasing relative humidity decreases both in-plane and out-of-plane elastic moduli.
Out-of-plane stiffness Ez exhibits heightened sensitivity to moisture fluctuations compared to in-plane moduli Ex and Ey.
Testing solid bleached board outside standard environmental limits distorts comparative modulus data. ISO 187 defines mandatory paper testing conditions at 23 degrees Celsius and 50 percent relative humidity. Moving a board sample from 50 percent to 80 percent relative humidity drops out-of-plane modulus Ez by up to 35 percent.
Moisture absorption causes fiber swelling across thickness, increasing sheet caliper while simultaneously softening fiber-to-fiber bond intersections.
Temperature rises also soften amorphous hemicellulose components. Laboratory temperature swings alter ultrasonic velocity measurements by roughly 0.2 percent per degree Celsius. Reliable property verification requires full thermal and moisture equilibration inside controlled environmental chambers before executing acoustic testing.

Furnish Composition and Refining Effects
Bleached softwood kraft fibers supply long-chain structural elements that form entanglements across ply boundaries. Bleached hardwood kraft fibers provide short, stiff building blocks that fill void spaces and increase sheet smooth surface profiles. Refining intensity directly influences out-of-plane density and bond network geometry.
High refining levels flatten tubular fibers into thin ribbons, increasing contact surface area between plies. Increased contact area elevates internal bond strength and increases out-of-plane elastic modulus Ez. Calendering operations pass wet-pressed sheets through heated steel rolls, compacting surface layers and increasing density. Hard nip calendering increases Ez at outer surfaces while maintaining bulk within uncalendered core zones.
Purchasing specifications require strict adherence to standardized conditioning schedules prior to lot acceptance.
- Pre-Conditioning Environment ~ Samples undergo low relative humidity drying at 20 to 35 percent relative humidity for 24 hours to eliminate moisture hysteresis history.
- Equilibrium Conditioning Environment ~ Samples maintain exposure to 23 degrees Celsius and 50 percent relative humidity for a minimum of 24 hours until weight changes stay under 0.1 percent over a 4-hour period.
- Specimen Handling Protocols ~ Operators wear clean cotton gloves to prevent moisture transfer from skin contact during acoustic testing preparation.
- Test Chamber Verification ~ Continuous recording calibrated hygrometers verify humidity stability within plus or minus 2 percent relative humidity tolerances.
Failure to condition samples according to ISO 187 rules nullifies mill certificate accuracy and voids seller defect liabilities. A single contract line requiring pre-conditioning before property verification alters lot acceptance thresholds by forcing all moisture history to a standardized baseline.

Valuation

Cost and Yield Mechanics in Down-Gauging
Paperboard purchase contracts price solid bleached board per metric tonne, but packaging converters sell finished cartons by unit count. Maximizing area yield per tonne of purchased substrate requires minimizing basis weight while preserving structural rigidity. Bending stiffness scales with the third power of thickness and linearly with in-plane elastic modulus.
Out-of-plane elastic parameters determine how well the sheet maintains thickness under converting stresses.
Lowering basis weight without losing caliper requires bulk-building strategy changes in inner plies. Inserting high-bulk mechanical pulp or unrefined hardwood kraft elevates overall sheet thickness per unit mass. This strategy lowers out-of-plane compressional modulus Ez. If Ez falls below critical converting thresholds, high-speed scoring rolls crush the sheet permanently, reducing finished package bending stiffness and risking high converting line reject rates.
| Substrate Option | Furnish Strategy | Ez Modulus | Delivered Cost per Tonne | Carton Yield per Tonne | Converting Reject Rate |
|---|---|---|---|---|---|
| Standard SBS 300 gsm | 100% Bleached Kraft Chemical Pulp | 280 MPa | 1,450 USD | 3,333 sheets | 0.8 percent |
| High-Bulk SBS 270 gsm | Softwood Outer / Mechanical Core | 190 MPa | 1,520 USD | 3,703 sheets | 1.5 percent |
| Ultra-Bulk SBS 250 gsm | Micro-Spheres / Hardwood Core | 140 MPa | 1,610 USD | 4,000 sheets | 4.2 percent |
| Dense SBS 320 gsm | Heavy Calendered Chemical Kraft | 340 MPa | 1,400 USD | 3,125 sheets | 0.3 percent |
Yield gains achieved by lower basis weights meet economic limits when internal crush occurs. High reject rates on packaging lines cancel out material savings from down-gauging. Calculating total landed cost requires factoring waste rates directly into sheet yield equations.

Delivered Cost Calculation Model
Assessing true packaging economy involves walking a job specification through material costs, waste factors, and run speeds. Consider a 50-tonne packaging production run.
Assume a standard 300 gsm solid bleached board lot costs 1,450 USD per metric tonne delivered. The job yields 3,333 parent sheets per tonne. Total raw material cost equals 72,500 USD for 166,650 sheets.
Processing at a 0.8 percent converting reject rate yields 165,316 usable sheets. Finished board cost lands at 438.55 USD per thousand usable sheets.
Substituting a down-gauged 270 gsm high-bulk option increases paper price to 1,520 USD per metric tonne due to specialty furnish costs. The 50-tonne purchase yields 185,150 parent sheets at a total cost of 76,000 USD. Lower out-of-plane modulus Ez increases creasing crushing defects, driving converting rejects up to 1.5 percent.
Usable sheet production reaches 182,372 sheets. Landed sheet cost drops to 416.73 USD per thousand usable sheets.
The down-gauged option saves 21.82 USD per thousand usable sheets despite higher raw material price per tonne and higher waste rates. Yield expansion dominates the cost equation when out-of-plane modulus remains sufficient to avoid massive line failures.
Choosing an ultra-bulk 250 gsm board with an Ez of 140 MPa pushes converting reject rates to 4.2 percent through fold line cracking and score crushing. Raw material cost rises to 1,610 USD per tonne, totaling 80,500 USD for 50 tonnes yielding 200,000 sheets. Usable production yields 191,600 sheets after rejecting crushed blanks.
Landed cost per thousand usable sheets rises to 420.15 USD while increasing machine downtime risks. Out-of-plane elastic property limits define the exact point where aggressive down-gauging destroys financial returns.
Mill technical datasheets highlight in-plane tensile strength and brightness figures while omitting out-of-plane elastic parameters. Board buyers must require ultrasonic Z-modulus figures in purchase specifications to protect carton structural integrity on high-speed converting lines.